Monitoring the Deposition of Copper Selenide Thin Films by Double Exposure Holographic Interferometry

 

V.P. Malekar and V.J. Fulari*

Holography and Materials Research Lab., Department of Physics, Shivaji University, Kolhapur, Maharashtra 416004, India.

*Corresponding Author E-mail: Vpyash07@gmail.com

 

ABSTRACT:

Double Exposure Holographic Interferometry (DEHI) is one of the most important applications of Holographic Interferometry. The reported technique, double exposure holographic interferometry used together with simple mathematical interpretation, which allow immediate finding of stress, mass, fringe width and thickness of thin film. It must be further noted that, fringe spacing changes with time of deposition as well as solution concentration. We have tested the samples for different normalities of solutions. The structural study was carried out by XRD for the conformation of material.

 

KEYWORDS: DEHI; Exposure; Stress; Fringe Width; Thin Film

 


 

1. INTRODUCTION:

Optical non destructive evaluation methods, using lasers as the object illumination source, include holographic interferometry. Holography is an interference method of recording the light waves diffracted by an object illuminated with coherent light. The diffracted waves are caused to interfere with a phase-related reference wave. If the waves are highly coherent the relative phase between subject and reference wave remains constant in time producing an observable effect on the intensity distribution of the resulting interference pattern. The photographic record of this pattern, called as hologram contains sufficient information about both, amplitudes (heights) of waves and phases (relative positions) of the waves reflected from the object1,2.

 

Copper selenide is semiconductor material which has a number of applications in solar cell, super ionic conductors, photo-detectors, etc3,4. Copper selenide usually exists as copper (I) selenide (Cu2Se or Cu2-XSe) or copper (II) selenide (CuSe or Cu3Se2). Copper (II) selenide in Cu3Se2 from in often reported as an impurity phase along with CuSe5,6.

 

Among the different deposition methods electrochemical deposition technique provides numerous advantages in comparison with all other methods.

 

The electrochemical method is very simple and because of its electric nature, the process can be controlled. In the present investigation we have synthesized CuSe thin films by electrodeposition technique and measured its thickness as well as stress to substrate by DEHI technique.

 

2. EXPERIMENTAL:

2.1 Thin film preparation:

CuSe thin films were prepared cathodically by electrodeposition technique on stainless steel substrate. Stainless steel substrate were mirror polished by zero grade polish paper and than ultrasonically cleaned with double distilled water. Electrolytic bath containing 0.10 M CuSO4 and 0.05 M SeO2 as a source of Cu and Se ions. Electrodeposition of CuSe thin films is carried out in potantiostatic mode. Pure graphite is used as an anode and stainless steel substrate is used as a cathode. For deposition potential measurement, saturated calomel electrode (SCE) is used as a reference electrode. Smooth, uniform and bluish-black colored CuSe thin films were obtained.

 

2.2. Double Exposure Holographic Interferometry (DEHI) technique :

The Double exposure holographic interferometry (DEHI) technique is used for thickness and stress measurement of CuS thin films. Fig.1. shows the experimental setup for recording hologram of the thin film. Light from the laser source is passed through beam splitter. The part of light (50%) is transmitted and incident on mirror, it illuminates the stainless steel substrate. The light scattered from stainless steel substrate is taken on holographic plate, which is called as object beam. The part of light (50%) reflected and incident on another mirror. It is directly incident on holographic film, which is reference beam. Initially steel substrate was recorded on holographic film as an object without deposition of the film. Secondly the holographic film was exposed by depositing CuS thin film for few seconds. It is reconstructed as that of the recording position in the path of reference beam, localized fringes are observed on the surface of substrates7.

3. RESULTS AND DISCUSSION:

3.1 Recording of hologram by DEHI:

Fig.2, 3 and 4 shows the holograms of CuSe thin films recorded on holographic film for deposition time 5sec, 10sec, 15sec, 20sec, 25sec for (0.05 M CuSO4 + 0.025 M SeO2),  (0.10 M CuSO4 + 0.050 M SeO2) and (0.15 M CuSO4 + 0.075 M SeO2) bath concentration. From Table 1, it is observed that as the time of deposition increases, the number of fringes localized on the surface of stainless steel substrate increases so fringe width decreases consequently thickness of film as well as mass deposited increases and stress to substrate decreases10. The variation of thickness with deposition time for different concentrations of CuSe thin films are shown in Fig.5 and the variation of stress with deposition time for different concentrations of CuSe thin films are shown in Fig.6. Also, Fig.7 gives variation of fringe width with deposition time for different concentrations of CuSe thin films are shown. Fig.8, 9 and 10 shows the variation of thickness of film, stress to substrate and mass of the film against fringe width of as-deposited CuSe thin films.

 

Fig.2. Holograms of CuSe thin film for a bath concentration (0.05 M CuSO4 + 0.025 M SeO2)  for deposition time (a) 5 s; (b) 10 s; (c) 15 s; (d) 20 s; (e) 25 s.

 

3.2. Fringe width:

From the table 1 it is clear that, as the deposition time as well as bath concentration increases, fringe width decreases. The fringe width decreases because of increase in thickness of CuSe thin films. The fringe width of recorded holograms of as-deposited CuSe thin films is measured by using traveling microscope.


Table 1 Thickness, mass and stress of CuSe thin

Bath Concen-

tration

Deposition

Time(sec)

Number of fringes

Thickness of CuSe film (μm)

Mass deposited (mg)

Stress×109

(dyne/cm2)

Fringe Width

(cm)

0.05M CuSO4

+

0.025M

SeO2

5

2

0.63

1.59

0.151

0.247

10

4

1.26

3.18

0.075

0.167

15

5

1.58

3.97

0.060

0.138

20

6

1.89

4.77

0.050

0.121

25

7

2.21

5.57

0.043

0.109

0.10M CuSO4

+

0.05M

SeO2

5

3

0.94

2.38

0.101

0.156

10

4

1.26

3.18

0.075

0.132

15

6

1.89

4.77

0.050

0.117

20

8

2.53

6.36

0.037

0.086

25

10

3.16

7.95

0.030

0.057

0.15M CuSO4

+

0.075M

SeO2

5

5

1.58

3.97

0.060

0.140

10

7

2.21

5.57

0.043

0.126

15

9

2.84

7.16

0.033

0.112

20

10

3.16

7.95

0.030

0.064

25

12

3.79

9.55

0.025

0.048

 

 

 

 

 

 

 

 


 

3.3. X-ray diffraction:

X-ray diffraction pattern of CuSe thin films of bath concentration (a) 0.05 M CuSO4 + 0.025 M SeO2, (b) 0.10 M CuSO4 + 0.050 M SeO2 and (c) 0.15 M CuSO4 + 0.075 M SeO2 on stainless steel substrate is shown in fig.11. Film is polycrystalline with orthorhombic. The observed d values are perfectly match with standard d values11, recorded in Table 2.

 

Table 2 Comparison of observed and standard‘d’ values of CuSe thin films

Obs.

No.

Standard ‘d’ values (A0)

Reflecting (hkl) Plane

Observed ‘d’

value (A0)

1

2.707

024

2.719

2

2.010

027

2.077

3

1.825

118

1.800

 

3.4. FT-Raman spectroscopy:

Raman spectra of the films were collected on a combination system including research grade FTIR model VERTEX 70 with model- Ram- II FT Raman spectrometer equipped with Nd-YAG laser at 1064nm wavelength. The spectra were recorded at laser power 0- 450 mW, the wave number range from 200- 4000 cm-1. The Raman spectra of CuSe film was shown in Fig.4.7 for bath concentration (a) 0.05 M CuSO4 + 0.025 M SeO2 (b) 0.10 M CuSO4 + 0.05 M SeO2 (c) 0.15 M CuSO4 + 0.075 M SeO2. The Raman band is at around 3187 cm-1.

 

4. CONCLUSIONS:

In this investigation CuSe films were prepared by a simple electrodeposition method in aqueous medium. Thickness, mass, stress to substrate and fringe width of the thin film can be measured by Double Exposure Holographic Interferometry technique. XRD study shows that the CuSe film is orthorhombic with polycrystalline in nature. From the holographic study, it is clear that, increase in concentration of precursors as well as deposition time, thickness, mass and number of fringes of the film increases but stress to the substrate and fringe width decreases. FT-Raman peak of CuSe shows at around 3187 cm-1.

 

5. REFERENCES:

1.       S.B. Gurevich, V.B. Konstantinov, J. Opt. Technol. 10 (1996) 3.

2.       S.J. Pawar, P.P. Chikode, V.J. Fulari, M.B. Dongare, Mater. Sci. Eng. B 37 (2007) 232.

3.       H. Okimura, T.Matsumae, R. Makabe, Thin Solid Films 71 (1980) 53.

4.       W. S. Chen, J. M. Stewart, R. A. Mickelson, Appl. Phys. Lett. 46 (1985) 1095.

5.       R. B. Shafizade, I. V. Ivanova, M. M. Kazinets, Thin Solid Films 55 (1978)     211.

6.       C. A. Estrada, P. K. Nair, M. T. S. Nair, R. A. Zingaro, E. A. Meyers, J electrochem. Soc. 141 (1994) 802.

7.       G. W. Stroke, An introduction of Coherent Optics and Holography, Academic Press, New York, (1969) 423.

8.       V. B. Prabhune, N. S. Shinde, V. J. Fulari, Appl. Surf. Sci. 255 (2008) 1819.

9.       P. P. Chikode, S. J. Pawar V. J. Fulari, M. B. Dongare, J. Opt. 36 (2007) 157.

10.     V. B. Prabhune, V. J. Fulari, Opt. Comm. 282 (2009) 2118.

11.     JCPDS data file No: 86-1239.

 

 

 

Received on 01.10.2009        Modified on 09.01.2010

Accepted on 20.03.2010        © AJRC All right reserved

Asian J. Research Chem. 3(3): July- Sept.  2010; Page 566-570